Diluting Isopon
 
Hi all

Some time ago, I took the advice of someone on this group to use Isopon for
critical filling work.
It works really well for tricky/exposed dents in wooden doors etc.
The only issue I have with the stuff is that, as you get to the last 1/3 of
the tin, it tends to have lost a lot of the liquid content and so becomes
difficult to mix and apply.
The tin I have has probably been in use for 9 months and opened maybe a
dozen times (I always put the top back on as soon as I have removed the
filler).

So what is the liquid and is there an alternative usually found in the
average garage cupboard?

TIA

Phil



1501 September 21st 09 08:57 AM

Diluting Isopon
 
On 21 Sep, 08:51, "TheScullster" wrote:
Hi all

Some time ago, I took the advice of someone on this group to use Isopon for
critical filling work.
It works really well for tricky/exposed dents in wooden doors etc.
The only issue I have with the stuff is that, as you get to the last 1/3 of
the tin, it tends to have lost a lot of the liquid content and so becomes
difficult to mix and apply.
The tin I have has probably been in use for 9 months and opened maybe a
dozen times (I always put the top back on as soon as I have removed the
filler).

So what is the liquid and is there an alternative usually found in the
average garage cupboard?

TIA

Phil


I've successfully thinned this type polyester filler with a drop of
polyester resin. (The type you use for GRP lay-up).

Stuart Noble September 21st 09 10:36 AM

Diluting Isopon
 
1501 wrote:
On 21 Sep, 08:51, "TheScullster" wrote:
Hi all

Some time ago, I took the advice of someone on this group to use Isopon for
critical filling work.
It works really well for tricky/exposed dents in wooden doors etc.
The only issue I have with the stuff is that, as you get to the last 1/3 of
the tin, it tends to have lost a lot of the liquid content and so becomes
difficult to mix and apply.
The tin I have has probably been in use for 9 months and opened maybe a
dozen times (I always put the top back on as soon as I have removed the
filler).

So what is the liquid and is there an alternative usually found in the
average garage cupboard?

TIA

Phil


I've successfully thinned this type polyester filler with a drop of
polyester resin. (The type you use for GRP lay-up).


Me too. Halfords do it in small cans, but it increases the setting time
a little IME

Roger Mills September 21st 09 11:28 AM

Diluting Isopon
 
In an earlier contribution to this discussion,
TheScullster wrote:

Hi all

Some time ago, I took the advice of someone on this group to use
Isopon for critical filling work.
It works really well for tricky/exposed dents in wooden doors etc.
The only issue I have with the stuff is that, as you get to the last
1/3 of the tin, it tends to have lost a lot of the liquid content and
so becomes difficult to mix and apply.
The tin I have has probably been in use for 9 months and opened maybe
a dozen times (I always put the top back on as soon as I have removed
the filler).

So what is the liquid and is there an alternative usually found in the
average garage cupboard?

TIA

Phil


Blimey, can you still get it?!

I remember using it (called David's Isopon then, ISTR) nearly 50 years ago
for repairing a corrugated iron water butt which had frozen solid, and the
ice had started to push the bottom out. Mavellous stuff - the butt lasted
another 20 years after that!
--
Cheers,
Roger
______
Email address maintained for newsgroup use only, and not regularly
monitored.. Messages sent to it may not be read for several weeks.
PLEASE REPLY TO NEWSGROUP!



Limey Lurker September 21st 09 10:39 PM

Diluting Isopon
 
On 21 Sep, 08:51, "TheScullster" wrote:
Hi all

Some time ago, I took the advice of someone on this group to use Isopon for
critical filling work.
It works really well for tricky/exposed dents in wooden doors etc.
The only issue I have with the stuff is that, as you get to the last 1/3 of
the tin, it tends to have lost a lot of the liquid content and so becomes
difficult to mix and apply.
The tin I have has probably been in use for 9 months and opened maybe a
dozen times (I always put the top back on as soon as I have removed the
filler).

So what is the liquid and is there an alternative usually found in the
average garage cupboard?

TIA

Phil




Next time you buy a can, make sure that you stir the contents every
time you use it; that way you'll get consistent density and setting
times.


All times are GMT +1. The time now is 06:20 PM.